内蒙古某高硫高碳铅锌矿新型抑制剂及捕收剂选矿试验研究

谢兰馨1,2,3 胡团柳1,2,3 张慧婷1,2,3 赖春华1,2,3 王泰存1,2,3 李荣康1,2,3   

  1. 1.西部矿业集团科技发展有限公司,青海 西宁 810006;2.青海省有色矿产资源工程技术研究中心,青海 西宁 810006; 3.青海省高原矿物加工工程与综合利用重点实验室,青海 西宁 810006
  • 出版日期:2026-07-15 发布日期:2026-07-15
  • 作者简介:谢兰馨(1997—),女,工程师。
  • 基金资助:
    青海省创新平台建设专项(编号:2022-ZJ-Y09)。

Experimental Study on a Novel Depressant and Collector for a High-Sulfur High-Carbon Lead-Zinc Ore in Inner Mongolia

XIE Lanxin1,2,3 HU Tuanliu1,2,3 ZHANG Huiting1,2,3 LAI Chunhua1,2,3 WANG Taicun1,2,3 LI Rongkang1,2,3   

  1. 1.Western Mining Group Science and Technology Development Co.,Ltd.,Xining 810006,China; 2.Qinghai Province Nonferrous Mineral Resources Engineering Technology Research Center,Xining 810006,China; 3.Key Laboratory of Plateau Mineral Processing Engineering and Comprehensive Utilization in Qinghai Province,Xining 810006,China
  • Online:2026-07-15 Published:2026-07-15

摘要: 针对高硫、高碳、微细粒嵌布的铅锌矿在高碱抑硫浮铅工艺中因石灰应用带来的管道结垢、贵金属回收 率低、回水处理成本高等问题,本研究以内蒙古某高硫高碳铅锌矿为对象,在工艺矿物学研究基础上,开发了适用于 低碱条件下磁黄铁矿的高效抑制剂XKY-02及对方铅矿具有高选择性的捕收剂XK-201。通过实验室小型闭路试验, 采用“铅优先浮选”工艺流程(一次粗选、两次扫选、粗精矿再磨后四次精选),在低碱药剂制度下获得了铅品位 56.44%、银品位260.55 g/t、铅回收率76.58%、银回收率45.29%的铅精矿。与常规高碱工艺相比,铅回收率提高 5.39个百分点,银回收率提高7.61个百分点,矿浆环境明显改善,且明显提高了锌精矿指标、减少了石灰及铅捕收剂 用量,经济与环境价值非常显著。该低碱工艺为高硫高碳难选铅锌矿的高效利用提供了新的技术途径。

关键词: 低碱工艺 , 方铅矿 , 磁黄铁矿 , 捕收剂 , 抑制剂

Abstract: To address the challenges associated with lime application in the high alkali sulfur suppression lead flotation process for high-sulfur,high-carbon,and finely disseminated lead-zinc ores—such as pipeline scaling,low precious metal recov ery,and high wastewater treatment costs—this study focuses on a high-sulfur,high-carbon lead-zinc ore from Inner Mongolia. Based on process mineralogy research,a highly efficient depressant XKY-02 for pyrrhotite and a highly selective collector XK 201 for galena were developed for low-alkalinity conditions.Laboratory-scale closed-circuit tests were conducted using a "lead preferential flotation" process consisting of one stage of roughing,two stages of scavenging,and four stages of cleaning after re grinding of the rough concentrate.Under the optimal low-alkalinity reagent regime,a lead concentrate with a lead grade of 56.44%,silver grade of 260.55 g/t,lead recovery of 76.58%,and silver recovery of 45.29% was obtained.Compared with the conventional high-alkalinity reagent regime,the lead recovery increased by 5.39 percentage points and the silver recovery in creased by 7.61 percentage points.The low-alkalinity process significantly improved the pulp environment,notably enhanced the zinc concentrate index,and effectively reduced the consumption of lime and lead collector,demonstrating significant eco nomic and environmental benefits.This low-alkalinity process provides a new technical approach for the efficient utilization of refractory high-sulfur,high-carbon lead-zinc ores.

Key words: low-alkalinity process,galena,pyrrhotite,collector,depressant