欢迎访问《金属矿山》杂志官方网站,今天是 分享到:
×

扫码分享

金属矿山 ›› 2015, Vol. 44 ›› Issue (02): 160-165.

• 安全与环保 • 上一篇    下一篇

大厂锡石多金属硫化矿尾矿中锰锌砷的溶出规律

刘奕祯1,莫伟2,张旭源1,马少健2,吴伯增3,陈锦全4   

  1. 1.广西大学环境学院,广西 南宁 530004;2.广西大学资源与冶金学院,广西 南宁 530004;3.广西有色 金属集团有限公司,广西 南宁 530022;4.广西华锡集团股份有限公司,广西 柳州 545006
  • 出版日期:2015-02-15 发布日期:2015-07-29
  • 基金资助:

    * 广西科技开发重大专项(编号:桂科重1298002-5),广西八桂学者科技项目(编号:HX01652013070022 )。

Release Law of Manganese,Zinc and Arsenic out of Cassiterite Polymetallic Sulfide Ore Tailings in Dachang

Liu Yizhen1,Mo Wei2,Zhang Xuyuan1,Ma Shaojian2,Wu Bozeng3,Chen Jinquan4   

  1. 1.School of Environment,Guangxi University,Nanning 530004,China;2.School of Resources and Metallurgy,Guangxi University,Nanning 530004,China;3.Guangxi Non-ferrous Metals Group Co. ,Ltd.,Nanning 530022,China;4.Guangxi Huaxi Group Co.,Ltd.,Liuzhou 545006,China
  • Online:2015-02-15 Published:2015-07-29

摘要: 广西大厂凤凰选矿厂处理锡石硫化矿。通过柱式静态浸泡试验研究了浸泡液初始pH值、液固比、尾矿堆积 高度对该厂尾矿中Mn、Zn、As溶出行为的影响以及不同条件下浸泡液pH的变化情况。结果表明:① 不同的 初始pH、液固比以及尾矿堆积高度下,随着浸泡时间的延长,Mn和Zn的溶出浓度均先显著下降然后趋于稳 定,累积溶出量均先快速增长然后缓慢增长,As则无论是溶出浓度还是累积溶出量均总体上呈近乎线性增 长趋势,而浸泡液的pH值均被中和到7.2~8.0之间。② 初始pH为3.5时Mn、Zn最易溶出,为5.5时次之,为 4.5时相对最难,但初始pH对As的溶出无显著影响;液固比越大,Mn、Zn和As均越容易溶出;尾矿堆积高度 总体上对Mn、Zn和As的溶出都无显著影响。③ 试验范围内,Mn、Zn、As的溶出量都很低,对应的累积溶出 量最大值分别只有14.505、13.471、0.768 mg/kg。以上研究成果可为现场尾矿库重金属污染的防控提供参 考。

关键词: 锡石硫化矿尾矿, 柱式静态浸泡, 浸泡液初始pH, 液固比, 尾矿堆积高度, 重金属溶出行为

Abstract: Fenghuang Dressing Plant of Dachang in Guangxi Province is planning to deal with the cassiterite sulfide ore.Effects of soaking solution pH,liquid-solid ratio,stack height on release behavior of Mn,Zn,As in tailings,as well as pH values at various conditions,are investigated through the column static soaking immersion tests.Results indicated that: ①when the initial pH,liquid-solid ratio,and stack height are different,and as the leaching time extended,release concentration of Mn and Zn is dropped dramatically first and then went steady.The cumulative release was rapidly increased first and then grown slowly.Meanwhile,As leaching concentration as well as cumulative release are nearly linearly increased,and the pH value of the soaking solution is neutralized from 7.2 to 8.0.②Mn and Zn releases are the easiest when the initial pH is 3.5,a little hard with pH value of 5.5,and the hardest when pH is 4.5,but the initial pH value has no influence on As leaching behavior; The higher of liquid-solid ratio,the more easily Mn,Zn and As is leached; Stack height of tailings has little influence on leaching behavior of Mn,Zn and As.③Within the test range,the release of Mn is very low,as well as Zn and As,and the corresponding maximum leaching amount is 14.505,13.471,0.768 mg/kg respectively.The research results above provide some references for heavy metal pollution prevention and control in the field of tailings dam.

Key words: Cassiterite sulfide ore tailings, Column static soaking, Initial pH of soaking solution, Liquid-solid ratio, Stack height of tailings, Heavy metals leaching behavior