浙江某复杂难选银多金属矿石选矿试验

毛益林1,2,杨进忠1,2,陈晓青1,2,严伟平1,2,王秀芬1,2   

  1. 1.中国地质科学院矿产综合利用研究所,四川 成都 610041;2.中国地质调查局金属矿产资源综合利用技术研究中心,四川 成都 610041
  • 出版日期:2015-03-15 发布日期:2015-07-31

Beneficiation Experiment Research on a Complex and Refractory Silver-Polymetallic Ore in Zhejiang Province

Mao Yilin1,2,Yang Jinzhong1,2,Chen Xiaoqing1,2,Yan Weiping1,2,Wang Xiufen1,2   

  1. 1.Institute of Multipurpose Utilization of Mineral Resources,Chinese Academy of Geological Sciences,Chengdu 610041,China;2.Research Center of Metal Mineral Resources Multipurpose Utilization,China Geological Survey,Chengdu 610041,China
  • Online:2015-03-15 Published:2015-07-31

摘要: 浙江某银多金属矿石银、铜、铅、锌含量分别为153 g/t、0.29%、0.83%、1.41%,铜、铅、锌主要以硫化物形式存在,主要有用矿物黄铜矿、方铅矿、闪锌矿之间以及与毒砂之间连生紧密,嵌布粒度粗细不均且形状不规则。为高效开发利用该矿石资源,在工艺矿物学研究基础上进行了选矿试验研究。试验结果表明,在磨矿细度为-0.045 mm占91.4%的情况下,采用1粗4精1扫铜铅混浮、铜铅混合精矿1粗2精2扫抑铅浮铜、混浮尾矿1粗4精2扫、中矿顺序返回流程处理,可取得铜品位为22.47%、银品位为1 373 g/t、铜回收率为69.08%、银回收率为8.02%的铜精矿,铅品位为40.63%、银品位为6 585 g/t、铅回收率为81.14%、银回收率为71.64%的铅精矿,锌品位为41.72%、银品位为197 g/t、锌回收率为79.85%、银回收率为3.48%的锌精矿。试验闭路流程是该矿石高效开发利用流程。

关键词: 银多金属矿, 铜铅混合浮选, 抑铅浮铜, 铜铅分离

Abstract: The silver-polymetallic ore in Zhejiang contains 153 g/t silver,0.29% copper,0.83% lead,1.41% zinc.Copper,lead,and zinc exist mainly in form of sulfide.Main valuable minerals,chalcopyrite,galenite,sphalerite,and dalarnite keep closely intergrowth with each other in uneven grain size and irregular shape.In order to high efficiently utilize the ore,beneficiation experiment was carried out based on the process mineralogy.The experiment results indicated that:at the grinding fineness of 91.4% passing 0.045 mm,and by adopting the process of copper-lead bulk flotation with one roughing-four cleaning-one scavenging,rough concentrate through one roughing-two cleaning-two scavenging lead depressing and copper floating,rough tailings through one roughing-four cleaning-two scavenging operation,and middles back to the flow-sheet in turn,copper concentrate with copper grade of 22.47%,silver grade of 1 373 g/t,copper recovery of 69.08%,silver recovery of 8.02%,lead concentrate with lead grade of 40.63%,silver grade of 6 585 g/t,lead recovery of 81.14%,silver recovery of 71.64%,and zinc concentrate with zinc grade of 41.72%,silver grade of 197 g/t,zinc recovery of 79.85%,silver recovery of 3.48% were obtained respectively.This experimental closed circuit process is high efficient in the development and utilization of the ore.

Key words: Silver polymetallic ore, Copper-lead bulk flotation, Lead depressing and copper floating, Copper separation from lead