缅甸某低品位复杂难选铁锡矿石综合回收试验研究

田小松1,2 武立伟1,3 赵 洵1,2 梁泽跃1,2 戴惠新1,4 吕玉辰1,4 王飞旺1,3   

  1. 1. 昆明理工大学国土资源工程学院,云南 昆明 650093;2. 云南迪庆有色金属有限责任公司,云南 迪庆 674401; 3. 矿物加工科学与技术国家重点实验室,北京 102268;4. 云南省金属矿尾矿资源二次利用工程研究中心,云南 昆明 650093
  • 出版日期:2024-04-15 发布日期:2024-05-17

Experimental Study on Comprehensive Recovery of a Low-grade Complex Refractory Iron and Tin Ore in Myanmar

TIAN Xiaosong1,2 WU Liwei1,3 ZHAO Xun1,2 LIANG Zeyue1,2 DAI Huixin1,4 #br# LÜ Yuchen1,4 WANG Feiwang1,3#br#   

  1. 1. Faculty of Land Resource Engineering,Kunming University of Science and Technology,Kunming 650093,China; 2. Yunnan Diqing Non-ferrous Metals Co. ,Ltd. ,Diqing 674401,China;3. Funded by Open Foundation of State Key Laboratory of Mineral Processing,Beijing 102268,China;4. Nationaland Local Joint Engineering Research Center for Green Comprehensive Utilizationof Metal Tailings Resources,Kunming 650093,China
  • Online:2024-04-15 Published:2024-05-17

摘要: 缅甸某低品位铁锡矿石含铁29. 79%、锡0. 495%,脉石成分主要为SiO2,主要有价矿物为磁铁矿和锡 石,二者紧密共生,粒度较细。为确定该矿石的高效开发利用工艺,基于原矿性质研究,采用湿式弱磁选铁—锡石回收 (摇床重选—摇床中矿再磨后高梯度强磁选除铁—摇床重选)—锡综合粗精矿浮选脱硫磁选除铁(弱磁选+高梯度强 磁选)流程进行了选矿试验。结果表明:该工艺最终可获得锡品位57. 956%、锡回收率69. 08%的锡精矿,铁品位 65. 21%、铁回收率48. 22%的铁精矿,硫品位46. 35%、硫回收率38. 31%的硫精矿,铁、锡和硫精矿所含杂质均未超标, 总尾矿的锡品位降至0. 153%,实现了铁锡矿石资源的综合回收利用。

关键词: 难选铁锡矿 弱磁选 高梯度磁选 摇床重选 再磨再选

Abstract: A low-grade iron tin ore in Myanmar contains iron of 29. 79% and tin of 0. 495%,and the gangue composition is mainly SiO2. The main valuable minerals are magnetite and cassite,which are closely symbiosis,and the grain size is fine. In order to determine the efficient development and utilization process of the ore,based on the study of raw ore properties,the process flow of wet low-intensity magnetic separation (LIMS) for iron selection,cassiterite recovery (shaking table gravity separation (STGS),high gradient magnetic separation (HGMS) after middle ore regrinding for iron removal and STGS),flotation desulphurization,magnetic separation for iron removal with tin comprehensive roughing concentrate(LIMS+HGMS) process was obtained for beneficiation experimental research. The results showed that the whole process closed-circuit test finally obtained tin concentrate with a tin grade of 57. 956% and recovery rate of 69. 08%,iron concentrate with an iron grade of 65. 21% and recovery rate of 48. 22%,sulfur concentrate with sulfur grade of 46. 35% and recovery rate of 38. 31%. The impurities contained in three kinds of concentrate products,such as iron,tin and sulfur,are not exceeded,and the tin grade of the total tailings is reduced to 0. 153%,which realizes the comprehensive recovery and utilization of iron tin ore resources.

Key words: refractory iron-tin ore,low-intensity magnetic separation,high gradient magnetic separation,shaker reselection, regrinding and reselection