欢迎访问《金属矿山》杂志官方网站,今天是 分享到:
×

扫码分享

金属矿山 ›› 2012, Vol. 41 ›› Issue (11): 145-147.

• 综合利用 • 上一篇    下一篇

某氰化尾渣直接还原焙烧—磁选选铁试验

刘娜,孙体昌,刘真真,蒋曼   

  1. 北京科技大学土木与环境工程学院
  • 出版日期:2012-11-15 发布日期:2012-11-27

Experiment of Iron Concentration From a Cyanided Tailing with the Process of Direct Reduction Roast-Magnetic Separation

Liu Na,Sun Tichang,Liu Zhenzhen,Jiang Man   

  1. Civil and Environmental Engineering Institute,University of Science and Technology Beijing
  • Online:2012-11-15 Published:2012-11-27

摘要: 对铁品位高达48.05%的某氰化尾渣进行了直接还原焙烧—磁选试验研究。结果表明,在烟煤2用量为20%,还原温度为1 150 ℃,还原时间为40 min,还原产物磨矿细度为-0.074 mm占78%,1次弱磁选磁场强度为87.56 kA/m情况下获得了铁品位为94.11%、回收率为90.14%的还原铁粉。该工艺不仅高效地富集了铁,而且使硫等含量较高的有害成分富集到了尾矿中。

关键词: 氰化尾渣, 直接还原焙烧, 磁选, 还原铁粉

Abstract: Experimental research on cyanided tailings containing 48.05% grade of iron by the process of direct reduction roast-magnetic separation tests was carried out. The results indicated that under the condition of roasting at 1 150  ℃ for 40 min with 20% bituminous coal 2,and grinding fineness of -0.074 mm 78% and magnetic intensity,the DRI with Fe grade of 94.11% and recovery of 90.14% was obtained by the process of one roughing low intensity magnetic separation with intensity of 87.56 kA/m. In the process,iron was concentrated efficiently,meanwhile high content of harmful ingredients,sulfur are enriched into tailings.

Key words: Cyanided tailings, Direct reducing roast, Magnetic separation, Direct reduction iron