四川某高钙型低品位硫化铅锌矿浮选试验

郭 姚1,2 ,徐龙华1,2 ,甘建强1,2 ,王志远1,2 ,苏 超1,2 ,吴 鑫1,2 ,冯海菊1,2 ,李国欢1,2 ,田 佳1,2 ,薛 凯1,2 ,罗 毅1,2   

  1. 1.西南科技大学环境与资源学院,四川 绵阳 621010; 2.西南科技大学固体废物处理与资源化教育部重点实验室,四川 绵阳 621010
  • 出版日期:2026-09-15 发布日期:2026-10-15
  • 通讯作者: 徐龙华(1987—),男,教授,博士,博士研究生导师。
  • 作者简介:郭 姚(1995—),女,博士研究生。
  • 基金资助:
    国家自然科学基金项目(编号:52425406);“十四五”国家重点研发计划项目(编号:2021YFC2900800);四川省科技计划项目(编号: 2023NSFSC1978);西南科技大学研究生创新基金项目(编号:25ycx3006)。

Flotation Test of a High-Calcium Low-Grade Lead-Zinc Sulfide Ore in Sichuan Province

GUO Yao1,2 ,XU Longhua1,2 ,GAN Jianqiang1,2 ,WANG Zhiyuan1,2 ,SU Chao1,2 ,WU Xin1,2 ,FENG Haiju1,2 ,LI Guohuan1,2 ,TIAN Jia1,2 ,XUE Kai1,2 ,LUO Yi1,2   

  1. 1.School of Environment and Resources,Southwest University of Science and Technology,Mianyang 621010,China; 2.Key Laboratory of Solid Waste Treatment and Resource Recycle,Ministry of Education,Southwest University of Science and Technology,Mianyang 621010,China
  • Online:2026-09-15 Published:2026-10-15

摘要: 四川某硫化铅锌矿石属低品位高钙型难选矿石,铅、锌品位分别为1.41%和8.12%,主要以硫化物形式 存在。由于铅品位低、含钙脉石矿物含量高,常规浮选难以实现铅锌有效分离回收。为实现该矿石的高效开发利用, 开展了浮选分离试验。采用优先浮选工艺,以自主研发的YTH为捕收剂,硫酸锌和亚硫酸钠为组合抑制剂,通过浮选 条件试验确定工艺流程和药剂制度。结果表明,采用“优先浮铅—铅尾矿再选锌”全流程闭路试验,铅、锌浮选均采用 1次粗选、1次扫选和3次精选,可获得铅品位63.57%、铅回收率75.52%、钙含量0.19%的铅精矿,以及锌品位 57.37%、锌回收率73.62%、钙含量0.74%的锌精矿。该工艺实现了低品位高钙型硫化铅锌矿石的有效开发利用,可 为同类型矿石的实际生产提供指导。

关键词: 硫化铅锌矿 , 高钙型矿石 , 浮选分离 , 优先浮选 , 含钙脉石 , YTH

Abstract: A lead-zinc sulfide ore from Sichuan is a low-grade,high-calcium refractory ore,with lead and zinc grades of 1.41% and 8.12%,Respectively;Lead and zinc mainly occur as sulfides.Due to the low lead grade and high content of calci um-bearing gangue minerals,conventional flotation cannot achieve effective separation and recovery of lead and zinc.To achieve efficient development and utilization of this ore,flotation separation tests were carried out.A preferential flotation process was a dopted,with self-developed YTH as the collector and zinc sulfate and sodium sulfite as combined depressants.The process flowsheet and reagent regime were determined through flotation condition tests.The results showed that a full-process closed circuit test using the flowsheet of "preferential lead flotation and zinc flotation from lead flotation tailings",in which both lead and zinc flotation adopted one roughing,one scavenging,and three cleaning stages,yielded a lead concentrate with a lead grade of 63.57%,a lead recovery of 75.52%,and a calcium content of 0.19%,as well as a zinc concentrate with a zinc grade of 57.37%,a zinc recovery of 73.62%,and a calcium content of 0.74%.This process achieved the effective development and u tilization of low-grade,high-calcium lead-zinc sulfide ore and can provide guidance for the industrial production of similar ores.

Key words: sulfide lead-zinc ore,high-calcium ore,flotation separation,preferential flotation,calcium-bearing gangue, YTH

中图分类号: